Troubleshooting
Tungsten contamination: why the arc wanders and how to stop it
A contaminated electrode does not usually fail all at once. It starts as a wandering arc, a dull tip and difficult re-starts — and ends as a tungsten inclusion in the weld. Working backwards from the symptom is faster than changing electrodes at random.
Where contamination actually comes from
- Tip contact. Dipping the electrode into the molten pool, or touching it with the filler rod, deposits base metal and filler alloy straight onto the hot tip.
- Base metal condition. Mill scale, oil, paint, zinc coating or aluminium oxide that was not removed before welding vaporises into the arc and condenses on the tip.
- Shielding gas faults. Flow set too low or too high, a leaking hose, a cracked gas lens, draughts at the bench, or post-flow that ends before the tip has cooled. Air reaches the hot tungsten and it oxidises.
- Wrong polarity or too much current for the diameter. The tip overheats, melts back and picks up material from the pool. An electrode running well over its current range degrades in minutes.
- Grinding residue. A wheel also used for steel embeds iron particles in the tungsten; grinding across the tip rather than along its axis leaves grooves that trap contamination.
What you see at the arc
- Arc cone becomes diffuse or wanders instead of staying tight and directional.
- The tip discolours, grows a crust, or balls up on DC work where a ground point is expected.
- Harder re-starts, sputtering on initiation, a grey or black sooty zone beside the bead.
- Tungsten inclusions in the weld — dense indications on radiography, or a hard spot that chatters when the joint is machined.
Once tungsten has entered the weld pool it cannot be burned out. The affected section has to be ground out and re-welded, which is why prevention is cheaper than troubleshooting.
A fix sequence that works
- Stop and cut back. Break off or grind away the contaminated 5–10 mm, then re-grind a clean point. Do not try to weld through a dirty tip.
- Clean the joint. Degrease and remove oxide mechanically from both faces and the filler rod; use a stainless-steel wire brush dedicated to the alloy.
- Verify the gas. Confirm the cylinder, regulator, hose connections and gas lens; set flow to the procedure, shield the work from draughts, and keep post-flow long enough for the tip to cool under gas.
- Match polarity and current. DCEN for steel and most DC work; check the selected amperage against the electrode diameter and tip angle.
- Separate the grinding setup. A dedicated fine-grit wheel or belt for tungsten only, grinding longitudinally with a consistent included angle.
- Only then change the electrode type. If low-current starting is still unreliable, a ceriated or lanthanated electrode starts more easily than pure tungsten at the same current — see our electrode selection guide.
Prevention checklist for the bench
| Control | What to check |
|---|---|
| Electrode size | Diameter matches the current range; ground to a consistent h7 finish |
| Tip preparation | Dedicated wheel, longitudinal grind, no cross grooves |
| Shielding | Correct gas, flow per WPS, intact gas lens, adequate post-flow |
| Workpiece | Oil, scale, oxide and coating removed before striking the arc |
| Handling | Clean gloves, tips protected in the pack, no contact with the pool or filler rod |
Why this matters when you buy electrodes
Consistent diameter, a clean ground surface and reliable colour marking per ISO 6848 make the first arc start predictable and reduce the temptation to push current beyond the electrode's range. For designation mapping between ISO 6848 and AWS A5.12, see the cross-reference guide on our sister site. Our size and amperage tables list the standard diameters and lengths we supply.
Frequently asked questions
Does a contaminated electrode have to be thrown away?
Rarely. Cut back the affected length and re-grind a clean point. Discard only if the contamination has travelled far up the electrode or the electrode has split.
Why does a brand-new electrode blacken on the first arc?
Almost always gas or polarity: insufficient shielding, no post-flow, a leaking line, or AC/DC set the wrong way for the electrode type. Check these before suspecting the electrode.
Is a black tip the same problem as a tungsten inclusion?
No. A black, oxidised tip is a surface condition you can grind away. An inclusion is tungsten metal already deposited in the weld and must be removed mechanically.